Academic Journal

The Effect of Collagen Removal and the Use of a Low-Viscosity Resin Liner on Marginal Adaptation of Resin Composite Restorations with Margins in Dentin.

التفاصيل البيبلوغرافية
العنوان: The Effect of Collagen Removal and the Use of a Low-Viscosity Resin Liner on Marginal Adaptation of Resin Composite Restorations with Margins in Dentin.
المؤلفون: Montes, M. A. J. R., de Goes, M. F., Ambrosano, G. M. B., Duarte, R. M., Sobrinho, L. C.
المصدر: Operative Dentistry; Jul/Aug2003, Vol. 28 Issue 4, p378-387, 10p
مصطلحات موضوعية: COLLAGEN, DENTIN, POLYMERIZATION, DENTAL caries
مستخلص: The study evaluated the influence of collagen removal and the use of a low-viscosity liner on the marginal quality of composite restorations for the total-etch system, Prime & Bond 2.1 (PB) and the self-etching primer system, Clearfil SE Bond (CSEB), in high C-factor cavities with margins in dentin. High C-factor cavities were made on dentin exposed from ground labial surfaces of 100 bovine lower incisors, randomly assigned to 10 treatment groups and restored with composite Z 250, placed in bulk. In Group 1 (PB), control group, PB was applied according to the manufacturer's directions; in Group 2 (PB/SH) following acid-etching, the surfaces were treated with 10% sodium hypochlorite (SH) for one minute and in Group 4 (PB/SH/PLF), the same procedure was conducted as for Group 3, plus an intermediate layer of PLF was applied as for Group 2. In Group 5 (CSEB), the control group, CSEB was applied according to the manufacturer's directions; in Group 6 (CSEB/PLF), an intermediate layer of PLF was applied; in Group 7 (SH/CSEB), the cavity surface was pre-treated with SH; in Group 8 (SH/CSEB/PLF), SH pre-treatment was conducted as for Group 7, then an intermediate layer of PLF was applied; in Group 9 (CSEB/SH), after CSEB-primer application, the surface was treated with SH, followed by CSEB-adhesive application and in Group 10 (CSEB/SH/PLF), the same was conducted as for Group 9, then an intermediate layer of PLF was applied. The specimens were stored at 37°C for 24 hours, polished, molded and replicas were obtained in epoxy resin. The replicas were gold-sputter coated and observed by SEM (300x) for marginal quality classification. The Kruskal-Wallis non-parametrical multi-comparison Test (p<0.05) was used to obtain statistical analysis of the data. Results demonstrated that both adhesive systems in the control groups presented low marginal quality and a high variability. The use of an intermediate layer of PLF significantly improved the marginal quality with the CSEB system but had no effect with the PB system. Collagen depletion with SH enhanced marginal quality for the PB system and did not influence the CSEB system results. [ABSTRACT FROM AUTHOR]
Copyright of Operative Dentistry is the property of Operative Dentistry and its content may not be copied or emailed to multiple sites or posted to a listserv without the copyright holder's express written permission. However, users may print, download, or email articles for individual use. This abstract may be abridged. No warranty is given about the accuracy of the copy. Users should refer to the original published version of the material for the full abstract. (Copyright applies to all Abstracts.)
قاعدة البيانات: Supplemental Index